Kilns and Firing

Pinholes and Blisters: A Firing-Schedule Fix

Pinholes and blisters are the same event caught at different moments: gas pushing up through molten glaze. A pinhole is a hole the glaze never healed over. A blister is a bubble that inflated and then burst or froze while still standing. Most cases are fixed by bisquing hotter and slower, applying glaze thinner, and adding a hold at peak with a controlled cool — in that order.

Tell them apart first, because the fixes differ

 PinholesBlisters
What you seeNeedle-fine holes through an otherwise smooth glaze, sometimes in scattered clustersRaised bumps, or open craters with sharp glassy rims, often 2–10 mm across
WhereAnywhere, but more on thicker glaze and on horizontal surfacesThick applications, insides of bowls, and over dark or copper-bearing glazes
Usual causeGas escaped late; glaze too stiff or cooled too fast to close the holeToo much gas at once, or overfiring boiling the glaze
Feels likeRough to a fingernail, glaze layer otherwise intactSharp, can cut — never food safe as-is

Neither is crawling, which is a bare patch where glaze pulled away before it melted, and neither is crazing, which is a fine crack network from glaze fit. If you have those, they have different causes entirely.

Where the gas comes from

Four sources, and you need to know which one is yours.

  • The clay body. Organic matter, carbon and sulfates burn out roughly between 570°F and 1650°F. If they are still burning out when the glaze has sealed over, the gas has to force its way through. Dark, iron-rich and heavily grogged bodies outgas more.
  • The glaze itself. Carbonates decompose and release carbon dioxide as they melt — whiting, dolomite, and especially copper carbonate and manganese dioxide, which are notorious for blistering when used heavily.
  • Application. Air trapped under the glaze layer: a bisque so dry and porous that it grabs the glaze and traps air, a fast dip that leaves bubbles, or brushed glaze applied over a partly dried coat.
  • Contamination. Soap or detergent residue in a sponge or bucket foams in the glaze and produces a fine, even scatter of pinholes that no schedule change will fix.

Bisque temperature is the most common culprit

Cone 06 is a popular bisque, and for many clay bodies it is not hot enough. It leaves organics and carbon still in the body, and those finish burning out in the glaze firing — underneath a sealed glaze layer.

Bisquing to cone 04 instead, slowly, deals with a large share of pinholing. The trade-off is that a hotter bisque is less porous, so the pot absorbs less glaze and you need to dip slightly longer or the layer comes out thin.

Slow matters as much as hot. Give the burnout zone real time rather than racing to temperature. A workable bisque:

  • 80°F/hr to 250°F, hold one hour if the work is at all damp
  • 150°F/hr to 1000°F
  • 100°F/hr from 1000°F to 1700°F — this is the burnout range, do not rush it
  • 150°F/hr to cone 04 (about 1945°F), hold 10–15 minutes

The glaze firing change that fixes most of the rest

Glaze needs time in its molten state to heal over the holes gas leaves behind, and it needs to not be boiling when you reach top temperature. Two adjustments do both.

Slow the last stretch and hold. Approaching peak at about 108°F/hr, then holding 10–20 minutes, gives the melt time to flatten out. Cones measure heat work, not temperature, so remember that a hold adds heat work — if a glaze starts running, shorten the hold or drop the peak slightly.

Control the cool. Dropping fast to about 1900°F and then cooling slowly, around 150°F/hr, down to roughly 1400°F keeps the glaze fluid long enough to close and smooth. A cone 6 schedule that works:

  • 150°F/hr to 220°F
  • 400°F/hr to 2000°F
  • 108°F/hr to cone 6 (about 2230°F), hold 10–15 minutes
  • Cool at full speed to 1900°F
  • Cool 150°F/hr to 1400°F, then off

If ramps and holds are new to you, our guide to firing schedules for beginners explains what each segment is doing.

The diagnostic sequence

Change one thing at a time, or you will never know what worked.

  • 1. Name the defect. Pinholes point at outgassing and healing. Blisters point at too much gas, overfiring, or a suspect material.
  • 2. Refire one affected piece at the same cone with a hold and a slow cool. If it heals, your problem is the schedule and you are done. If the same spots reopen in the same places, the gas is coming from the body or the application. Refiring is a legitimate test as well as a repair.
  • 3. Raise the bisque to cone 04 and slow the burnout range. Fire the same glaze on the same body and compare.
  • 4. Thin the glaze. Thick glaze gives gas further to travel and more to heal. Halve your application on a test piece.
  • 5. Look at the recipe. Heavy copper carbonate, manganese, or a very high carbonate load blisters on its own. Blisters that appear only under one glaze are a glaze problem, not a kiln problem.
  • 6. Check for contamination — new sponges, a bucket washed with detergent, hand lotion on bisque ware.

What to do with the pieces you already have

  • Pinholed but smooth: refire with a hold and slow cool. Often it closes completely.
  • Blistered with sharp edges: grind the sharp glass down with a diamond pad first, then reglaze the ground area and refire. Refiring over unground blisters usually reproduces them.
  • Pinholes only on food-contact surfaces: do not use it as is. Holes hold bacteria and the body underneath is exposed.
  • One piece in an otherwise clean load: suspect that piece — contamination, thick glaze, or a spot you handled with greasy hands — not the kiln.

Frequently asked questions

How do I fix pinholes in glaze?

Bisque to cone 04 slowly, apply glaze thinner, and add a 10–15 minute hold at peak with a controlled cool from 1900°F down to 1400°F. Refiring an existing pinholed piece on that schedule often heals it.

Will refiring fix blisters?

Sometimes, but only if you grind the sharp edges flat first and, ideally, touch in a little glaze. A blister refired untouched tends to blister again in the same place.

Is pinholed pottery food safe?

Not on food-contact surfaces. The holes are hard to clean and expose the clay body. On the outside of a vase or the back of a tile it is a cosmetic problem only.

Can bisquing too hot cause pinholes?

Indirectly. A very hot bisque reduces porosity so much that the glaze goes on thin and unevenly, which brings its own defects. Cone 04 is the usual balance for a cone 6 body.

Why do I only get pinholes on the inside of bowls?

Glaze pools thicker on horizontal surfaces, and gravity holds the escaping gas against the glaze longer. Thin the application inside forms, and lean harder on the hold and slow cool.

If the schedule fix does not hold, the glaze itself may be the problem — a fluid, carbonate-heavy or copper-rich glaze will blister no matter how carefully you fire it. Browse glaze suppliers in the PotteryList directory to find stable commercial glazes tested at your cone, and work through firing schedules for beginners before you change three things at once.

Benefit art show and sale

Hope in Bloom: benefit art show and sale for West Cancer Foundation

Thursday, December 10, 3:30 to 6:30 pm at Tucker Collective in Memphis. Free admission. Proceeds support West Cancer Foundation.

Event details ›

Sponsored by The Potter's Hands Studio

Get The Kiln Log

New pottery studios, classes and upcoming pottery events, once a week.

Search